Worked example
Example: Kraft 47 %, 2 % rejects. The inputs, in the units selected above:
| Input | Value |
|---|---|
| Total pulp yield on OD wood | 47.000 % |
| Rejects (share of total pulp) | 2.0000 % |
| Basic density of the wood (OD mass per green volume) | 450.00 kg/m³ |
Applying the formula below gives:
| Result | Value |
|---|---|
| Screened yield | 46.060 % |
| OD wood per air-dry tonne of pulp | 1.9540 kg/kg |
| Solid wood per air-dry tonne | 4.3422 m³/t |
Open this example in the calculator and change any input.
Formula
\(Y_s = Y(1 - r), \quad W_{OD} = \frac{0.9}{Y_s}, \quad V_w = \frac{W_{OD}}{\rho_b}\)
Variables
| Symbol | Meaning | SI unit |
|---|---|---|
| \(Y\) | Total pulp yield on OD wood | - |
| \(r\) | Rejects (share of total pulp) | - |
| \(\rho_b\) | Basic density of the wood (OD mass per green volume) | kg/m³ |
| \(Y_s\) | Screened yield | - |
| \(W_{OD}\) | OD wood per air-dry tonne of pulp | kg/kg |
| \(V_w\) | Solid wood per air-dry tonne | m³/kg |
Method and standards
Yield definitions.
Where it is used
- Wood procurement.
- Mill yield monitoring.
Common mistakes
- Mixing OD and AD tonnes.
- Using air-dry density for green volume.
Assumptions and limits
- Rejects not re-cooked.
- Wood consumption is for screened chips to the digester; bark, fines and chip-screening losses are not included.
References
- Smook
- Handbook for Pulp & Paper Technologists
- 3rd ed. (Angus Wilde, 2002)
- ch. 4 and 8: yield on wood; air-dry ton = 90 % bone-dry fibre and 10 % water (ch. 8)
Questions and answers
What yields are typical?
Kraft 45–50 %, sulphite 45–55 %, mechanical pulps 90–97 %.
What is an air-dry tonne?
0.9 t of bone-dry fibre plus 0.1 t of water.
Why basic density?
Wood is bought by volume; basic density converts solid cubic metres to OD tonnes.
Method and article reviewed by FireCAD engineering on 13 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.