Worked example
Example: Illustrative steel, Cr-Ka {211}, tension. The inputs, in the units selected above:
| Input | Value |
|---|---|
| X-ray wavelength | 2.2900 Å |
| Peak position at ψ = 0 | 156.40 ° |
| Peak position at tilt ψ | 156.00 ° |
| Tilt angle | 45.000 ° |
| Elastic modulus (diffraction value) | 210.00 GPa |
| Poisson's ratio | 0.29000 - |
Applying the formula below gives:
| Result | Value |
|---|---|
| Lattice spacing at ψ = 0 | 1.1697 Å |
| Lattice spacing at ψ | 1.1706 Å |
| Strain difference (d_ψ − d₀)/d₀ | 735.87 µε |
| Residual stress (tension positive) | 239.59 MPa |
Open this example in the calculator and change any input.
Formula
\(d = \frac{\lambda}{2\sin\theta}, \quad \sigma_\phi = \frac{E}{1 + \nu}\,\frac{d_\psi - d_0}{d_0\sin^2\psi}\)
Variables
| Symbol | Meaning | SI unit |
|---|---|---|
| \(\lambda\) | X-ray wavelength | m |
| \(2\theta_0\) | Peak position at ψ = 0 | rad |
| \(2\theta_\psi\) | Peak position at tilt ψ | rad |
| \(\psi\) | Tilt angle | rad |
| \(E\) | Elastic modulus (diffraction value) | Pa |
| \(\nu\) | Poisson's ratio | - |
| \(d_0\) | Lattice spacing at ψ = 0 | m |
| \(d_\psi\) | Lattice spacing at ψ | m |
| \(\varepsilon_\psi\) | Strain difference (d_ψ − d₀)/d₀ | - |
| \(\sigma_\phi\) | Residual stress (tension positive) | Pa |
Method and standards
Residual stress.
Where it is used
- Checking shot peening, grinding and welding stresses.
- Quality control of surface treatments.
Common mistakes
- Using bulk instead of diffraction elastic constants.
- Ignoring ψ-splitting from shear stresses.
Assumptions and limits
- Biaxial surface stress; two-tilt method; homogeneous material.
References
- X-ray diffraction sin²ψ method
Questions and answers
Why use high-angle peaks?
The peak shift for a given strain is largest near 2θ = 180°, so high-angle reflections give the best sensitivity.
How deep does the measurement reach?
Only a few micrometres in steel; it is a surface stress, and layers are removed electrolytically to profile depth.
What do the defaults represent?
An illustrative ferritic steel measurement with Cr-Kα radiation (2.29 Å) on the {211} peak near 156°, shifting 0.4° at a 45° tilt.
Method and article reviewed by FireCAD engineering on 17 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.
Sources
Noyan and Cohen, Residual Stress: Measurement by Diffraction and Interpretation (Springer, 1987), Callister and Rethwisch, Materials Science and Engineering: An Introduction (Wiley)