FireCADCalc

Creep Stress Relaxation of a Bolt or Constrained Part

Stress remaining after a time in a part held at constant total strain (bolted joint, spring) relaxing by Norton power-law creep, and the time to half stress.

Inputs

Examples: Illustrative alloy-steel bolt, 10,000 hFast-relaxing spring, n = 3Nickel alloy bolt, n = 8

Accepted: 0.1 to 5,000 MPa
Accepted: 0.1 to 1,000 GPa
Accepted: 3.6E-17 to 3,600 1/h
Accepted: 1.01 to 20
Accepted: 0 to 2,777,800 h

Results

At constant total strain, elastic strain converts into creep strain: dσ/dt = −Eε̇ with ε̇ = ε̇₀(σ/σ₀)ⁿ (Norton). Integrating gives σ(t) = σ₀[1 + (n − 1)Eε̇₀t/σ₀]^(−1/(n−1)). Relaxation is fast at first and slows as stress falls, which is why bolts in hot flanges are retightened after the first heat-up. Primary creep, ignored here, makes early relaxation faster still.

Remaining stress117.44MPa
Fraction retained58.722%
Time to relax to half the initial stress1,578.9h
Creep strain accumulated434.51µε

Download PDF CSV Link to this result Compare another case

Log in to save calculations to your dashboard.

Worked example

Example: Illustrative alloy-steel bolt, 10,000 h. The inputs, in the units selected above:

InputValue
Initial stress300.00 MPa
Elastic modulus at temperature170.00 GPa
Creep rate at the initial stress1.0000e-08 1/h
Norton stress exponent5.0000 -
Time at temperature10,000 h

Applying the formula below gives:

ResultValue
Remaining stress285.06 MPa
Fraction retained95.021 %
Time to relax to half the initial stress661,765 h
Creep strain accumulated87.869 µε

Open this example in the calculator and change any input.

Formula

\(\sigma(t) = \sigma_0\left[1 + \frac{(n-1)E\dot\varepsilon_0t}{\sigma_0}\right]^{-1/(n-1)}\)

Variables

Symbol Meaning SI unit
\(\sigma_0\) Initial stress Pa
\(E\) Elastic modulus at temperature Pa
\(\dot\varepsilon_0\) Creep rate at the initial stress 1/s
\(n\) Norton stress exponent -
\(t\) Time at temperature s
\(\sigma(t)\) Remaining stress Pa
\(\sigma/\sigma_0\) Fraction retained -
\(t_{1/2}\) Time to relax to half the initial stress s
\(\varepsilon_c\) Creep strain accumulated -

Method and standards

Stress relaxation.

Where it is used

  • Hot flange and turbine casing bolting.
  • Springs and shrink fits at temperature.

Common mistakes

  • Using a creep rate at a different stress.
  • Ignoring the joint's own elastic follow-up (stiffer bolt relaxes faster).

Assumptions and limits

  • Secondary creep only; constant temperature; rigid joint (no follow-up).

References

  • Stress relaxation under Norton creep at constant strain

Questions and answers

Why retighten hot bolts?

Most of the relaxation happens early; restoring the preload once gives a longer service interval.

What creep rate should I use?

The secondary creep rate of the bolt material at the initial stress and service temperature.

What do the defaults represent?

An illustrative alloy-steel bolt at 300 MPa preload, 170 GPa hot modulus, 10⁻⁸/h initial creep rate, n = 5, after 10,000 h.

Method and article reviewed by FireCAD engineering on 17 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.

Sources

Dieter, Mechanical Metallurgy, SI metric ed. (McGraw-Hill, 1988)

Related calculators

Free engineering calculators: every page computes in SI and converts to your units. Results are for engineering estimation; verify critical designs against the referenced standards.

Rejoining the server...

Rejoin failed... trying again in seconds.

Failed to rejoin.
Please retry or reload the page.

The session has been paused by the server.

Failed to resume the session.
Please retry or reload the page.