Worked example
Example: Illustrative ceramic coating on steel strip. The inputs, in the units selected above:
| Input | Value |
|---|---|
| Coating elastic modulus | 200.00 GPa |
| Coating Poisson's ratio | 0.25000 - |
| Coating expansion coefficient | 8.0000 µm/(m·K) |
| Substrate expansion coefficient | 12.000 µm/(m·K) |
| Cooling from stress-free (deposition) temperature | 800.00 K |
| Coating thickness | 5.0000 µm |
| Substrate elastic modulus | 200.00 GPa |
| Substrate Poisson's ratio | 0.30000 - |
| Substrate thickness | 1.0000 mm |
Applying the formula below gives:
| Result | Value |
|---|---|
| Mismatch strain | 3,200.0 µε |
| Coating stress (compression negative) | -853.33 MPa |
| Substrate curvature | 0.089600 1/m |
| Radius of curvature | 11.161 m |
Open this example in the calculator and change any input.
Formula
\(\sigma_c = -\frac{E_c(\alpha_s - \alpha_c)\Delta T}{1 - \nu_c}, \quad \kappa = \frac{6\sigma_ct_c(1 - \nu_s)}{E_st_s^2}\)
Variables
| Symbol | Meaning | SI unit |
|---|---|---|
| \(E_c\) | Coating elastic modulus | Pa |
| \(\nu_c\) | Coating Poisson's ratio | - |
| \(\alpha_c\) | Coating expansion coefficient | 1/K |
| \(\alpha_s\) | Substrate expansion coefficient | 1/K |
| \(\Delta T\) | Cooling from stress-free (deposition) temperature | K |
| \(t_c\) | Coating thickness | m |
| \(E_s\) | Substrate elastic modulus | Pa |
| \(\nu_s\) | Substrate Poisson's ratio | - |
| \(t_s\) | Substrate thickness | m |
| \(\Delta\varepsilon\) | Mismatch strain | - |
| \(\sigma_c\) | Coating stress (compression negative) | Pa |
| \(\kappa\) | Substrate curvature | 1/m |
| \(R\) | Radius of curvature | m |
Method and standards
Coating stress.
Where it is used
- Thermal spray, PVD and enamel coatings.
- Thin films on wafers.
Common mistakes
- Omitting the biaxial factor 1/(1 − ν).
- Applying Stoney to thick coatings.
Assumptions and limits
- Thin elastic coating; uniform temperature; constant properties.
References
- Thin-film thermal stress and Stoney's equation
Questions and answers
Why do ceramic coatings spall on cooling?
Large compressive or tensile mismatch stresses, plus edge effects, exceed the interface toughness.
What else causes coating stress?
Intrinsic growth stresses from deposition (peening in PVD, quench stresses in thermal spray) add to the thermal part.
What do the defaults represent?
An illustrative 5 µm ceramic-like coating (α 8 µm/m·K) on a 1 mm steel strip (α 12 µm/m·K) cooled 800 K from deposition.
Method and article reviewed by FireCAD engineering on 17 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.
Sources
Ohring, Materials Science of Thin Films, 2nd ed. (Academic Press, 2002), Callister and Rethwisch, Materials Science and Engineering: An Introduction (Wiley)