Worked example
Example: 250 MPa on a 300 MPa, m 10 ceramic. The inputs, in the units selected above:
| Input | Value |
|---|---|
| Applied stress | 250.00 MPa |
| Characteristic strength (63.2 %) of the test volume | 300.00 MPa |
| Weibull modulus | 10.000 - |
| Stressed volume relative to the test volume | 1.0000 - |
| Target failure probability | 1.0000 % |
Applying the formula below gives:
| Result | Value |
|---|---|
| Failure probability at σ | 14.914 % |
| Stress for the target probability | 189.38 MPa |
Open this example in the calculator and change any input.
Formula
\(P_f = 1 - \exp\left[-\frac{V}{V_0}\left(\frac{\sigma}{\sigma_0}\right)^m\right], \quad \sigma_t = \sigma_0\left[\frac{-\ln(1 - P_t)}{V/V_0}\right]^{1/m}\)
Variables
| Symbol | Meaning | SI unit |
|---|---|---|
| \(\sigma\) | Applied stress | Pa |
| \(\sigma_0\) | Characteristic strength (63.2 %) of the test volume | Pa |
| \(m\) | Weibull modulus | - |
| \(V/V_0\) | Stressed volume relative to the test volume | - |
| \(P_t\) | Target failure probability | - |
| \(P_f\) | Failure probability at σ | - |
| \(\sigma_t\) | Stress for the target probability | Pa |
Method and standards
Weibull distribution.
Where it is used
- Ceramic components and refractories.
- Glass and brittle coatings.
Common mistakes
- Using a test-bar σ₀ for a large part without the size effect.
- Fitting m from too few tests.
Assumptions and limits
- Uniform stress; volume flaws. σ₀ from flexural tests belongs to the effective (stressed) volume of the test bar, which is much smaller than its geometric volume; using geometric volumes for a tensile part understates the size effect. Use effective volumes in V/V₀.
References
- Weibull (1951) weakest-link distribution P_f = 1 − exp[−(V/V₀)(σ/σ₀)^m] (Dowling, Mechanical Behavior of Materials, 4th ed. (Pearson, 2013), ch. 8)
Questions and answers
What does the modulus m mean?
How scattered the strength is: high m means consistent strength, low m means wide scatter and a large size effect.
Why does part size matter?
A bigger stressed volume is more likely to contain a large flaw, so its median strength is lower.
What do the defaults represent?
A ceramic with 300 MPa characteristic strength and modulus 10, loaded to 250 MPa.
Method and article reviewed by FireCAD engineering on 13 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.