Worked example
Example: Rougher-cleaner, cleaner tails to rougher. The inputs, in the units selected above:
| Input | Value |
|---|---|
| Circuit | Rougher–cleaner, cleaner tails to rougher feed |
| Stage 1 recovery of the valuable mineral (rougher or cleaner) | 92.000 % |
| Stage 2 recovery of the valuable mineral (cleaner or scavenger) | 85.000 % |
| Stage 1 recovery of gangue | 20.000 % |
| Stage 2 recovery of gangue | 30.000 % |
Applying the formula below gives:
| Result | Value |
|---|---|
| Circuit recovery of the valuable mineral | 90.719 % |
| Circuit recovery of gangue | 6.9767 % |
| Separation efficiency | 83.743 % |
| Circulating load of the valuable mineral (recycle / feed) | 16.009 % |
Open this example in the calculator and change any input.
Formula
\(R_{circ} = \frac{R_1R_2}{1 - R_1 + R_1R_2}\ (\text{rougher–cleaner}), \quad R_{circ} = \frac{R_1}{1 - R_2(1 - R_1)}\ (\text{cleaner–scavenger})\)
Variables
| Symbol | Meaning | SI unit |
|---|---|---|
| \(\text{circuit}\) | Circuit | - |
| \(R_{1A}\) | Stage 1 recovery of the valuable mineral (rougher or cleaner) | - |
| \(R_{2A}\) | Stage 2 recovery of the valuable mineral (cleaner or scavenger) | - |
| \(R_{1B}\) | Stage 1 recovery of gangue | - |
| \(R_{2B}\) | Stage 2 recovery of gangue | - |
| \(R_A\) | Circuit recovery of the valuable mineral | - |
| \(R_B\) | Circuit recovery of gangue | - |
| \(SE\) | Separation efficiency | - |
| \(CL_A\) | Circulating load of the valuable mineral (recycle / feed) | - |
Method and standards
Mass balance around a two-stage circuit.
Where it is used
- Flowsheet selection.
- Estimating the effect of an extra cleaner or scavenger.
Common mistakes
- Using circuit recoveries as stage recoveries.
- Forgetting the extra volume for the circulating load.
Assumptions and limits
- Recycle floats like fresh feed.
References
- Wills and Finch
- Wills' Mineral Processing Technology
- 8th ed. (Butterworth-Heinemann, 2016)
- ch. 10
- eqs. 10.5-10.6 and ch. 12
- eqs. 12.48-12.50
Questions and answers
Why recycle the cleaner tails?
They still hold valuable mineral; returning them gives it another chance and raises circuit recovery above the single-pass value.
What does the circulating load show?
How much valuable mineral cycles inside the circuit; high loads raise selectivity but need cell and pump capacity.
What do the defaults represent?
A rougher recovering 92 % of the mineral and 20 % of the gangue, and a cleaner recovering 85 % and 30 %.
Method and article reviewed by FireCAD engineering on 17 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.