Worked example
Example: Wills Example 3.8, zinc flotation (sphalerite). The inputs, in the units selected above:
| Input | Value |
|---|---|
| Feed assay (metal) | 3.9300 % |
| Concentrate assay | 52.070 % |
| Tailings assay | 0.49000 % |
| Feed rate (dry solids) | 100.00 t/h |
| Metal content of the valuable mineral | 67.098 % |
Applying the formula below gives:
| Result | Value |
|---|---|
| Yield (mass to concentrate) | 6.6693 % |
| Ratio of concentration | 14.994 |
| Enrichment ratio | 13.249 |
| Metal recovery to concentrate | 88.363 % |
| Concentrate rate | 6.6693 t/h |
| Tailings rate | 93.331 t/h |
| Gangue recovery to concentrate | 1.5866 % |
| Separation efficiency (Schulz) | 86.777 % |
Open this example in the calculator and change any input.
Formula
\(\frac{C}{F} = \frac{f - t}{c - t}, \quad R = \frac{C c}{F f}, \quad SE = R - R_g = \frac{C}{F}\frac{m(c - f)}{f(m - f)}\)
Variables
| Symbol | Meaning | SI unit |
|---|---|---|
| \(f\) | Feed assay (metal) | - |
| \(c\) | Concentrate assay | - |
| \(t\) | Tailings assay | - |
| \(F\) | Feed rate (dry solids) | kg/s |
| \(m\) | Metal content of the valuable mineral | - |
| \(C/F\) | Yield (mass to concentrate) | - |
| \(F/C\) | Ratio of concentration | - |
| \(c/f\) | Enrichment ratio | - |
| \(R\) | Metal recovery to concentrate | - |
| \(C\) | Concentrate rate | kg/s |
| \(T\) | Tailings rate | kg/s |
| \(R_g\) | Gangue recovery to concentrate | - |
| \(SE\) | Separation efficiency (Schulz) | - |
Method and standards
Two-product formula and Schulz separation efficiency.
Where it is used
- Daily metallurgical accounting in concentrators.
- Comparing operating conditions on a grade-recovery basis.
Common mistakes
- Mixing percent and fraction assays.
- Applying it to a circuit with more than two products.
Assumptions and limits
- Steady state; metal in one mineral.
References
- Wills and Finch
- Wills' Mineral Processing Technology
- 8th ed. (Butterworth-Heinemann, 2016)
- ch. 1
- eqs. 1.1-1.5 (Schulz, 1970) and ch. 3
- eqs. 3.23-3.27
- Examples 1.3 and 3.8
Questions and answers
Why use assays instead of weighing the products?
Concentrate and tailings flows are rarely weighed; the assays of three samples fix the split through the metal balance.
What is a good separation efficiency?
It is recovery of the valuable mineral less recovery of gangue; 100 % is a perfect separation and 0 % no separation at all.
What do the defaults represent?
Wills's Example 3.8: zinc flotation with 3.93 % Zn feed, 52.07 % concentrate and 0.49 % tailings (6.7 % yield, 88.4 % recovery).
Method and article reviewed by FireCAD engineering on 17 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.