Worked example
Example: Reference 13.0 kWh/t ore, test ore ground coarser. The inputs, in the units selected above:
| Input | Value |
|---|---|
| Work index of the reference ore | 13.000 kWh/t |
| Reference feed 80 % passing | 1,700.0 µm |
| Reference product 80 % passing | 140.00 µm |
| Test ore feed 80 % passing | 1,750.0 µm |
| Test ore product 80 % passing | 165.00 µm |
Applying the formula below gives:
| Result | Value |
|---|---|
| Work index of the test ore | 14.522 kWh/t |
| Energy input (same for both) | 7.8340 kWh/t |
| Hardness relative to the reference | 1.1171 |
Open this example in the calculator and change any input.
Formula
\(W_{it} = W_{ir}\frac{10/\sqrt{P_{80r}} - 10/\sqrt{F_{80r}}}{10/\sqrt{P_{80t}} - 10/\sqrt{F_{80t}}}\)
Variables
| Symbol | Meaning | SI unit |
|---|---|---|
| \(W_{ir}\) | Work index of the reference ore | J/kg |
| \(F_{80r}\) | Reference feed 80 % passing | m |
| \(P_{80r}\) | Reference product 80 % passing | m |
| \(F_{80t}\) | Test ore feed 80 % passing | m |
| \(P_{80t}\) | Test ore product 80 % passing | m |
| \(W_{it}\) | Work index of the test ore | J/kg |
| \(W\) | Energy input (same for both) | J/kg |
| \(W_{it}/W_{ir}\) | Hardness relative to the reference | - |
Method and standards
Equal energy in Bond's equation for both ores.
Where it is used
- Ore variability programmes.
- Checking a laboratory work index.
Common mistakes
- Grinding different masses of the two ores.
- Using a reference ore of unknown index.
Assumptions and limits
- Same mill, time and mass for both ores.
References
- Wills and Finch
- Wills' Mineral Processing Technology
- 8th ed. (Butterworth-Heinemann, 2016)
- ch. 5
- eq. 5.8 (Berry and Bruce, 1966)
Questions and answers
Why not run the full Bond test?
The locked-cycle Bond test is slow; the comparative test needs one batch grind of each ore and a reference ore of known index.
What limits its accuracy?
The two products must have similar size distributions; very different ores break differently.
What do the defaults represent?
A reference ore of 13.0 kWh/t ground from 1,700 to 140 µm; the test ore went from 1,750 to 165 µm in the same time.
Method and article reviewed by FireCAD engineering on 17 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.