Worked example
Example: Illustrative steel in copper, 100 to 1. The inputs, in the units selected above:
| Input | Value |
|---|---|
| Cathodic current density on the noble metal | 5.0000e-07 A/mm² |
| Cathode (noble metal) area | 1.0000 m² |
| Anode (active metal) area | 0.010000 m² |
| Anode molar mass | 55.845 kg/kmol |
| Electrons per atom | 2.0000 - |
| Anode density | 7,870.0 kg/m³ |
Applying the formula below gives:
| Result | Value |
|---|---|
| Area ratio | 100.00 |
| Galvanic current | 0.50000 A |
| Anode current density | 50.000 A/m² |
| Anode penetration rate | 58.022 mm/a |
| Rate with equal areas | 0.58022 mm/a |
Open this example in the calculator and change any input.
Formula
\(i_a = i_c\frac{A_c}{A_a}, \quad CR = \frac{i_aM}{nF\rho}\)
Variables
| Symbol | Meaning | SI unit |
|---|---|---|
| \(i_c\) | Cathodic current density on the noble metal | A/m² |
| \(A_c\) | Cathode (noble metal) area | m² |
| \(A_a\) | Anode (active metal) area | m² |
| \(M\) | Anode molar mass | kg/kmol |
| \(n\) | Electrons per atom | - |
| \(\rho\) | Anode density | kg/m³ |
| \(A_c/A_a\) | Area ratio | - |
| \(I\) | Galvanic current | A |
| \(i_a\) | Anode current density | A/m² |
| \(CR\) | Anode penetration rate | m/s |
| \(CR_{1:1}\) | Rate with equal areas | m/s |
Method and standards
Area effect.
Where it is used
- Fastener and fitting material selection.
- Explaining failures at dissimilar joints.
Common mistakes
- Ignoring the area ratio.
- Painting only the anode.
Assumptions and limits
- Uniform current over each area; cathode reaction rate known.
References
- Mixed-potential area effect with Faraday's law
Questions and answers
Why is a small anode so bad?
The whole cathode's reaction is balanced by dissolution of a small area, concentrating the attack.
Why paint the cathode rather than the anode?
Painting the anode leaves small holidays as tiny anodes against a large cathode; painting the cathode cuts the cathodic area.
What do the defaults represent?
An illustrative 1 m² of copper with 0.5 A/m² oxygen reduction coupled to 0.01 m² of steel.
Method and article reviewed by FireCAD engineering on 17 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.
Sources
Fontana, Corrosion Engineering, 3rd ed. (McGraw-Hill, 1986)