Worked example
Example: Illustrative marine concrete, 50 mm cover. The inputs, in the units selected above:
| Input | Value |
|---|---|
| Concrete cover | 50.000 mm |
| Apparent chloride diffusion coefficient | 31.558 mm²/a |
| Surface chloride (by mass of binder) | 3.0000 % |
| Initial chloride | 0.10000 % |
| Critical (threshold) chloride | 0.40000 % |
| Service life to check | 50.000 a |
Applying the formula below gives:
| Result | Value |
|---|---|
| Corrosion initiation time | 14.938 a |
| Chloride at the rebar at the service life | 1.1830 % |
| Cover needed to reach the service life | 91.475 mm |
Open this example in the calculator and change any input.
Formula
\(C(x,t) = C_i + (C_s - C_i)\left[1 - \text{erf}\frac{x}{2\sqrt{D_at}}\right], \quad t_i = \frac{x^2}{4D_az^2}\)
Variables
| Symbol | Meaning | SI unit |
|---|---|---|
| \(x\) | Concrete cover | m |
| \(D_a\) | Apparent chloride diffusion coefficient | m²/s |
| \(C_s\) | Surface chloride (by mass of binder) | - |
| \(C_i\) | Initial chloride | - |
| \(C_{crit}\) | Critical (threshold) chloride | - |
| \(t_s\) | Service life to check | s |
| \(t_i\) | Corrosion initiation time | s |
| \(C(x, t_s)\) | Chloride at the rebar at the service life | - |
| \(x_{min}\) | Cover needed to reach the service life | m |
Method and standards
Chloride ingress.
Where it is used
- Durability design of marine and de-iced structures.
- Assessing remaining life of existing concrete.
Common mistakes
- Mixing chloride by mass of concrete and of binder.
- Using short-term D_a as constant for decades.
Assumptions and limits
- Constant D_a and surface chloride; one-dimensional diffusion; uncracked concrete.
References
- Fick's second law for chloride ingress (initiation period)
Questions and answers
Why does cover matter so much?
Initiation time grows with the square of cover depth.
What threshold should I use?
Often 0.2–0.4 % chloride by mass of binder for normal reinforcement; it depends on the concrete and exposure.
What do the defaults represent?
An illustrative marine-exposed concrete: 50 mm cover, D_a 1 × 10⁻¹² m²/s, 3 % surface chloride, 0.1 % initial and 0.4 % threshold, checked at 50 years.
Method and article reviewed by FireCAD engineering on 17 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.
Sources
Tuutti, Corrosion of Steel in Concrete (Swedish Cement and Concrete Research Institute, 1982), Fontana, Corrosion Engineering, 3rd ed. (McGraw-Hill, 1986)