FireCADCalc

CO₂ Corrosion Rate of Carbon Steel (de Waard–Milliams)

CO₂ corrosion rate of bare carbon steel from temperature and CO₂ partial pressure, with the protective-scale correction above the scaling temperature.

Inputs

Examples: Illustrative wet gas line at 60 C, 50 bar, 2 % CO2Hot line at 100 C with scale correctionSame hot line, worst case

Accepted: 0 to 150 °C
Accepted: 0.1 to 500 bar
Accepted: 0.001 to 100 %

Results

The de Waard–Milliams nomogram equation log V = 5.8 − 1710/T + 0.67 log p_CO₂ (V in mm/a, T in K, p in bar) gives the rate on bare steel in condensed water with no inhibitor or scale. Above the scaling temperature log T_scale = 2400/(6.7 + 0.6 log p_CO₂), protective iron carbonate forms and the rate falls by F_scale = 10^(2400/T − 0.6 log p − 6.7). Later versions add corrections for fugacity, pH, flow, glycol and oil wetting; treat this as a conservative screening rate.

CO₂ partial pressure1.0000bar
Nomogram corrosion rate4.6470mm/a
Scaling temperature85.059°C
Scale factor1.0000
Corrected corrosion rate4.6470mm/a

Download PDF CSV Link to this result Compare another case

Log in to save calculations to your dashboard.

Worked example

Example: Illustrative wet gas line at 60 C, 50 bar, 2 % CO2. The inputs, in the units selected above:

InputValue
Temperature60.000 °C
Total pressure50.000 bar
CO₂ mole fraction in the gas2.0000 %
Protective scale correctionApply above the scaling temperature

Applying the formula below gives:

ResultValue
CO₂ partial pressure1.0000 bar
Nomogram corrosion rate4.6470 mm/a
Scaling temperature85.059 °C
Scale factor1.0000
Corrected corrosion rate4.6470 mm/a

Open this example in the calculator and change any input.

Formula

\(\log V = 5.8 - \frac{1710}{T} + 0.67\log p_{CO_2}, \quad \log T_{scale} = \frac{2400}{6.7 + 0.6\log p_{CO_2}}\)

Variables

Symbol Meaning SI unit
\(T\) Temperature K
\(p\) Total pressure Pa
\(y_{CO_2}\) CO₂ mole fraction in the gas -
\(\text{scale}\) Protective scale correction -
\(p_{CO_2}\) CO₂ partial pressure Pa
\(V_{nom}\) Nomogram corrosion rate m/s
\(T_{scale}\) Scaling temperature K
\(F_{scale}\) Scale factor -
\(V\) Corrected corrosion rate m/s

Method and standards

CO₂ corrosion.

Where it is used

  • Corrosion allowance and inhibitor selection for oil and gas lines.
  • Material selection screening (carbon steel versus CRA).

Common mistakes

  • Using total pressure instead of CO₂ partial pressure.
  • Applying it where H₂S dominates (sour service).

Assumptions and limits

  • Bare steel, condensed water, no inhibitor; no flow or pH corrections.

References

  • de Waard–Milliams CO₂ corrosion model

Questions and answers

Why does the rate fall at high temperature?

Iron carbonate scale becomes protective above the scaling temperature, typically 60–80 °C.

Is this rate used directly for design?

It is a conservative screening value; inhibitor availability and flow corrections are applied in detailed models.

What do the defaults represent?

An illustrative wet gas line at 60 °C and 50 bar with 2 % CO₂.

Method and article reviewed by FireCAD engineering on 17 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.

Sources

de Waard, Lotz and Milliams, Predictive Model for CO2 Corrosion Engineering in Wet Natural Gas Pipelines, Corrosion 47 (1991); de Waard, Lotz and Dugstad, Corrosion 93 paper 69

Related calculators

Free engineering calculators: every page computes in SI and converts to your units. Results are for engineering estimation; verify critical designs against the referenced standards.

Rejoining the server...

Rejoin failed... trying again in seconds.

Failed to rejoin.
Please retry or reload the page.

The session has been paused by the server.

Failed to resume the session.
Please retry or reload the page.