Worked example
Example: Illustrative wet gas line at 60 C, 50 bar, 2 % CO2. The inputs, in the units selected above:
| Input | Value |
|---|---|
| Temperature | 60.000 °C |
| Total pressure | 50.000 bar |
| CO₂ mole fraction in the gas | 2.0000 % |
| Protective scale correction | Apply above the scaling temperature |
Applying the formula below gives:
| Result | Value |
|---|---|
| CO₂ partial pressure | 1.0000 bar |
| Nomogram corrosion rate | 4.6470 mm/a |
| Scaling temperature | 85.059 °C |
| Scale factor | 1.0000 |
| Corrected corrosion rate | 4.6470 mm/a |
Open this example in the calculator and change any input.
Formula
\(\log V = 5.8 - \frac{1710}{T} + 0.67\log p_{CO_2}, \quad \log T_{scale} = \frac{2400}{6.7 + 0.6\log p_{CO_2}}\)
Variables
| Symbol | Meaning | SI unit |
|---|---|---|
| \(T\) | Temperature | K |
| \(p\) | Total pressure | Pa |
| \(y_{CO_2}\) | CO₂ mole fraction in the gas | - |
| \(\text{scale}\) | Protective scale correction | - |
| \(p_{CO_2}\) | CO₂ partial pressure | Pa |
| \(V_{nom}\) | Nomogram corrosion rate | m/s |
| \(T_{scale}\) | Scaling temperature | K |
| \(F_{scale}\) | Scale factor | - |
| \(V\) | Corrected corrosion rate | m/s |
Method and standards
CO₂ corrosion.
Where it is used
- Corrosion allowance and inhibitor selection for oil and gas lines.
- Material selection screening (carbon steel versus CRA).
Common mistakes
- Using total pressure instead of CO₂ partial pressure.
- Applying it where H₂S dominates (sour service).
Assumptions and limits
- Bare steel, condensed water, no inhibitor; no flow or pH corrections.
References
- de Waard–Milliams CO₂ corrosion model
Questions and answers
Why does the rate fall at high temperature?
Iron carbonate scale becomes protective above the scaling temperature, typically 60–80 °C.
Is this rate used directly for design?
It is a conservative screening value; inhibitor availability and flow corrections are applied in detailed models.
What do the defaults represent?
An illustrative wet gas line at 60 °C and 50 bar with 2 % CO₂.
Method and article reviewed by FireCAD engineering on 17 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.
Sources
de Waard, Lotz and Milliams, Predictive Model for CO2 Corrosion Engineering in Wet Natural Gas Pipelines, Corrosion 47 (1991); de Waard, Lotz and Dugstad, Corrosion 93 paper 69