Cement Heat of Hydration from Bogue Composition

Heat of complete hydration of a cement from its Bogue compounds, and the adiabatic temperature rise of concrete for a cement content.

Inputs

Examples: Illustrative OPC, 350 kg/m3Low-heat cement, mass pourRapid-hardening cement

Accepted: 0 to 100 %
Accepted: 0 to 100 %
Accepted: 0 to 30 %
Accepted: 0 to 30 %
Accepted: 50,000,000 to 800,000,000 mg/Nm³
J/(m³·K); about 2.3–2.6 MJ/(m³·K).Accepted: 1,000,000 to 4,000,000

Results

Each clinker compound releases a characteristic heat on complete hydration: about 502 J/g for C₃S, 260 for C₂S, 867 for C₃A and 419 for C₄AF. Their weighted sum is the heat the cement can release; most of it comes in the first week, faster for fine, C₃S- and C₃A-rich cement. Multiplied by the cement content and divided by the concrete's volumetric heat capacity, it gives the upper bound of temperature rise in a large pour with no heat loss, used to judge thermal cracking risk. Blended cements release less.

Heat of complete hydration384.56kJ/kg
Adiabatic temperature rise of the concrete at complete hydration47.089K

Download PDF CSV Link to this result Compare another case

Log in to save calculations to your dashboard.

Worked example

Example: Illustrative OPC, 350 kg/m3. The inputs, in the units selected above:

InputValue
Tricalcium silicate58.000 %
Dicalcium silicate16.000 %
Tricalcium aluminate8.0000 %
Tetracalcium aluminoferrite10.000 %
Cement content of the concrete3.5000e+08 mg/Nm³
Volumetric heat capacity of the concrete2,400,000 -

Applying the formula below gives:

ResultValue
Heat of complete hydration444.02 kJ/kg
Adiabatic temperature rise of the concrete at complete hydration64.753 K

Open this example in the calculator and change any input.

Formula

\(H = 502\,C_3S + 260\,C_2S + 867\,C_3A + 419\,C_4AF\ \text{(J/g)}, \quad \Delta T_{ad} = \frac{H\,c}{\rho c_p}\)

Variables

Symbol Meaning SI unit
\(C_3S\) Tricalcium silicate -
\(C_2S\) Dicalcium silicate -
\(C_3A\) Tricalcium aluminate -
\(C_4AF\) Tetracalcium aluminoferrite -
\(c\) Cement content of the concrete kg/m³
\(\rho c_p\) Volumetric heat capacity of the concrete -
\(H\) Heat of complete hydration J/kg
\(\Delta T_{ad}\) Adiabatic temperature rise of the concrete at complete hydration K

Method and standards

Heat of hydration.

Where it is used

  • Mass concrete and thermal cracking checks.
  • Comparing cement types.

Common mistakes

  • Treating the complete-hydration heat as the early heat.
  • Ignoring supplementary materials in blended cement.

Assumptions and limits

  • Complete hydration; adiabatic concrete.

References

  • Heats of complete hydration of the clinker compounds

Questions and answers

How much heat does Portland cement release?

About 450–500 kJ/kg at complete hydration; about 70 % of it in the first week.

How hot can a mass pour get?

About 18 K per 100 kg/m³ of Portland cement at complete hydration with no heat loss; real pours rise less because hydration is incomplete in the first days and some heat escapes.

What do the defaults represent?

An illustrative OPC with 58 % C₃S, 16 % C₂S, 8 % C₃A and 10 % C₄AF in concrete with 350 kg/m³.

Method and article reviewed by FireCAD engineering on 17 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.

Sources

Taylor, Cement Chemistry, 2nd ed. (Thomas Telford, 1997)

Related calculators

Free engineering calculators: every page computes in SI and converts to your units. Results are for engineering estimation; verify critical designs against the referenced standards.

Rejoining the server...

Rejoin failed... trying again in seconds.

Failed to rejoin.
Please retry or reload the page.

The session has been paused by the server.

Failed to resume the session.
Please retry or reload the page.