Worked example
Example: 308L-type deposit. The inputs, in the units selected above:
| Input | Value |
|---|---|
| Chromium (wt %) | 19.500 % |
| Molybdenum (wt %) | 0.20000 % |
| Silicon (wt %) | 0.40000 % |
| Niobium (wt %) | 0 % |
| Nickel (wt %) | 10.000 % |
| Carbon (wt %) | 0.020000 % |
| Manganese (wt %) | 1.8000 % |
| Nitrogen (wt %) | 0.050000 % |
| Copper (wt %) | 0.10000 % |
Applying the formula below gives:
| Result | Value |
|---|---|
| Schaeffler Cr equivalent | 20.300 |
| Schaeffler Ni equivalent | 11.500 |
| WRC-1992 Cr equivalent | 19.700 |
| WRC-1992 Ni equivalent | 11.725 |
| WRC-1992 ratio | 1.6802 |
| Solidification mode (0 A, 1 AF, 2 FA, 3 F) | 2.0000 |
Open this example in the calculator and change any input.
Formula
\(Cr_{eq} = Cr + Mo + 0.7Nb,\quad Ni_{eq} = Ni + 35C + 20N + 0.25Cu\ (\text{WRC-1992})\)
\(Cr_{eq} = Cr + Mo + 1.5Si + 0.5Nb,\quad Ni_{eq} = Ni + 30C + 0.5Mn\ (\text{Schaeffler})\)
Variables
| Symbol | Meaning | SI unit |
|---|---|---|
| \(Cr\) | Chromium (wt %) | - |
| \(Mo\) | Molybdenum (wt %) | - |
| \(Si\) | Silicon (wt %) | - |
| \(Nb\) | Niobium (wt %) | - |
| \(Ni\) | Nickel (wt %) | - |
| \(C\) | Carbon (wt %) | - |
| \(Mn\) | Manganese (wt %) | - |
| \(N\) | Nitrogen (wt %) | - |
| \(Cu\) | Copper (wt %) | - |
| \(Cr_{eq,S}\) | Schaeffler Cr equivalent | - |
| \(Ni_{eq,S}\) | Schaeffler Ni equivalent | - |
| \(Cr_{eq,WRC}\) | WRC-1992 Cr equivalent | - |
| \(Ni_{eq,WRC}\) | WRC-1992 Ni equivalent | - |
| \(Cr_{eq}/Ni_{eq}\) | WRC-1992 ratio | - |
| \(\text{mode}\) | Solidification mode (0 A, 1 AF, 2 FA, 3 F) | - |
Method and standards
Equivalent formulas.
Where it is used
- Dissimilar welds (stainless to carbon steel).
- Filler selection for austenitic stainless.
Common mistakes
- Ignoring dilution from the base metal.
- Using Schaeffler for high-nitrogen alloys.
Assumptions and limits
- Weld metal compositions. The ferrite number is not computed: read it from the WRC-1992 diagram. The Schaeffler Ni equivalent leaves out nitrogen, so for high-nitrogen fillers the two methods can disagree.
References
- Schaeffler (1949) and WRC-1992 (Kotecki and Siewert) equivalent formulas; solidification-mode ratios from Lippold and Kotecki
- Welding Metallurgy and Weldability of Stainless Steels (Wiley, 2005)
Questions and answers
Why does ferrite matter in stainless welds?
A little ferrite (3–10 FN) during solidification absorbs sulphur and phosphorus and prevents hot cracking.
Why two formulas?
Schaeffler is the classic diagram; WRC-1992 adds nitrogen and copper and predicts ferrite better for modern fillers.
What do the defaults represent?
A 308L-type weld deposit.
Method and article reviewed by FireCAD engineering on 13 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.