Worked example
Example: Structural plate C 0.18 Mn 1.2 Si 0.3. The inputs, in the units selected above:
| Input | Value |
|---|---|
| Carbon | 0.18000 % |
| Manganese | 1.2000 % |
| Silicon | 0.30000 % |
| Chromium | 0.10000 % |
| Molybdenum | 0.050000 % |
| Vanadium | 0.020000 % |
| Nickel | 0.10000 % |
| Copper | 0.15000 % |
| Boron | 0 % |
Applying the formula below gives:
| Result | Value |
|---|---|
| Carbon equivalent (IIW) | 0.43067 % |
| Cracking parameter (Ito–Bessyo) | 0.26950 % |
Open this example in the calculator and change any input.
Formula
\(CE_{IIW} = C + \frac{Mn}{6} + \frac{Cr + Mo + V}{5} + \frac{Ni + Cu}{15}\)
\(P_{cm} = C + \frac{Si}{30} + \frac{Mn + Cu + Cr}{20} + \frac{Ni}{60} + \frac{Mo}{15} + \frac{V}{10} + 5B\)
Variables
| Symbol | Meaning | SI unit |
|---|---|---|
| \(C\) | carbon | mass % |
| \(Mn\) | manganese | mass % |
| \(Si\) | silicon | mass % |
| \(Cr\) | chromium | mass % |
| \(Mo\) | molybdenum | mass % |
| \(V\) | vanadium | mass % |
| \(Ni\) | nickel | mass % |
| \(Cu\) | copper | mass % |
| \(B\) | boron | mass % |
| \(CE_{IIW}\) | carbon equivalent | mass % |
| \(P_{cm}\) | cracking parameter | mass % |
Method and standards
IIW carbon equivalent and the Ito–Bessyo cracking parameter, both as given in EN 1011-2 Annex C.
Where it is used
- Welding procedure qualification.
- Repair welding of old steels.
- Material substitution checks.
Common mistakes
- Using specification maxima instead of actual analysis.
- Using CE(IIW) on low-carbon micro-alloyed steels.
- Forgetting boron in Pcm.
Assumptions and limits
- Steel analysis in mass %; formulas apply to carbon and low-alloy steels.
- CE and Pcm come out in mass % (shown as, for example, 0.43 %); codes quote the same number without the % sign (CE = 0.43).
References
- IIW carbon equivalent; Ito–Bessyo Pcm; EN 1011-2 Annex C
Questions and answers
What is CE for C 0.18, Mn 1.2, Si 0.3, Cr 0.1, Mo 0.05, V 0.02, Ni 0.1, Cu 0.15?
CE(IIW) 0.43 and Pcm 0.27.
Which one should I use?
CE(IIW) for most carbon–manganese steels; Pcm for low-carbon (under about 0.12 % C) high-strength steels.
Does CE give the preheat?
Not alone: the welding code combines it with thickness, hydrogen level and heat input.
Method and article reviewed by FireCAD engineering on 12 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.