Worked example
Example: 50 mm bar, 2 t/h, to 1250 C. The inputs, in the units selected above:
| Input | Value |
|---|---|
| Bar diameter | 50.000 mm |
| Production rate | 2,000.0 kg/h |
| Resistivity of the hot steel (above the Curie point) | 1.2000 Ω·mm²/m |
| Relative permeability (1 above the Curie point) | 1.0000 - |
| Required ratio of diameter to reference depth | 4.0000 - |
| Mean specific heat, ambient to final | 670.00 J/(kg·K) |
| Initial temperature | 20.000 °C |
| Final temperature | 1,250.0 °C |
| Overall coil efficiency | 65.000 % |
Applying the formula below gives:
| Result | Value |
|---|---|
| Minimum heat time | 96.875 s |
| Minimum coil line length | 3.3598 m |
| Lowest frequency for the D/δ ratio | 1.9454 kHz |
| Reference depth at that frequency | 12.500 mm |
| Power into the steel | 457.83 kW |
| Power at the coil terminals | 704.36 kW |
Open this example in the calculator and change any input.
Formula
\(t_{min} = 25D^2\ [\text{s, in}], \quad l_{min} = 0.03\,\dot m\ [\text{in, lb/h}], \quad f_{min} = \frac{\rho}{\pi\mu_0\mu_r(D/k)^2}, \quad P_w = \dot mc(T_f - T_{in})\)
Variables
| Symbol | Meaning | SI unit |
|---|---|---|
| \(D\) | Bar diameter | m |
| \(\dot m\) | Production rate | kg/s |
| \(\rho\) | Resistivity of the hot steel (above the Curie point) | Ω·m |
| \(\mu_r\) | Relative permeability (1 above the Curie point) | - |
| \(D/\delta\) | Required ratio of diameter to reference depth | - |
| \(c\) | Mean specific heat, ambient to final | J/(kg·K) |
| \(T_{in}\) | Initial temperature | K |
| \(T_f\) | Final temperature | K |
| \(\eta\) | Overall coil efficiency | - |
| \(t_{min}\) | Minimum heat time | s |
| \(l_{min}\) | Minimum coil line length | m |
| \(f_{min}\) | Lowest frequency for the D/δ ratio | 1/s |
| \(\delta\) | Reference depth at that frequency | m |
| \(P_w\) | Power into the steel | W |
| \(P_c\) | Power at the coil terminals | W |
Method and standards
The ballpark relations for inline bar heating.
Where it is used
- Preliminary design of forging heaters.
- Checking an existing line against a new bar size.
Common mistakes
- Using a frequency set for a larger bar.
- Taking the coil length as the heated length only.
Assumptions and limits
- Carbon steel; ambient to forging temperature; continuous feed.
Questions and answers
Why does the heat time grow with D²?
Heat must conduct from the induced surface layer to the centre; conduction time scales with the square of the distance.
Why choose the lowest efficient frequency?
Lower frequency puts the heat deeper and shortens the soak, but below D/δ ≈ 4 the currents cancel and efficiency collapses.
What do the defaults represent?
50 mm carbon steel bar at 2 t/h heated from 20 to 1,250 °C, resistivity 1.2 μΩ·m above the Curie point, mean specific heat 670 J/(kg·K), overall coil efficiency 65 %.
Method and article reviewed by FireCAD engineering on 17 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.
Sources
Rudnev, Loveless, Cook and Black, Handbook of Induction Heating (Marcel Dekker, 2003), sec. 7.1, eqs. 7.1 and 7.2 (ballpark heat time and coil length) and the D/δ > 4 rule; sec. 3.3.1 (power)