Worked example
Example: 0.05 % C at 1,600 C, 1 and 0.2 atm. The inputs, in the units selected above:
| Input | Value |
|---|---|
| Carbon content | 0.050000 % |
| CO partial pressure | 1.0000 atm |
| CO pressure under vacuum | 0.20000 atm |
| Melt temperature | 1,600.0 °C |
Applying the formula below gives:
| Result | Value |
|---|---|
| Equilibrium oxygen at p_CO | 400.00 ppm |
| Equilibrium oxygen at the vacuum CO pressure | 80.000 ppm |
| Oxygen solubility with liquid FeO | 0.22855 % |
| Carbon below which iron oxide forms (at p_CO) | 0.008751 % |
Open this example in the calculator and change any input.
Formula
\([\%C][\text{ppm O}] = 20\,p_{CO}, \quad \log[\%O]_{sat} = -\frac{6380}{T} + 2.765\)
Variables
| Symbol | Meaning | SI unit |
|---|---|---|
| \([\%C]\) | Carbon content | - |
| \(p_{CO}\) | CO partial pressure | Pa |
| \(p_{CO}'\) | CO pressure under vacuum | Pa |
| \(T\) | Melt temperature | K |
| \([O]\) | Equilibrium oxygen at p_CO | - |
| \([O]'\) | Equilibrium oxygen at the vacuum CO pressure | - |
| \([\%O]_{sat}\) | Oxygen solubility with liquid FeO | - |
| \([\%C]_{min}\) | Carbon below which iron oxide forms (at p_CO) | - |
Method and standards
Carbon-oxygen equilibrium in liquid iron.
Where it is used
- BOF and EAF end-point oxygen.
- Vacuum decarburisation of ultra-low-carbon steel.
Common mistakes
- Using it at high carbon without activity corrections.
- Entering p_CO in bar or kPa into the atm form.
Assumptions and limits
- Low-alloy steel below 1 % C; equilibrium, not kinetics.
Questions and answers
Why does vacuum help decarburisation?
C + O = CO(g): lowering p_CO shifts the equilibrium so that the same carbon coexists with less oxygen, and carbon reacts with the dissolved oxygen without adding more.
What is the oxygen saturation?
The highest oxygen liquid iron can hold before liquid iron oxide separates: about 0.23 % at 1,600 °C (Taylor and Chipman).
What do the defaults represent?
0.05 % C at 1,600 °C: 400 ppm O at 1 atm CO and 80 ppm at 0.2 atm; oxygen saturation is 0.23 %, so iron oxide forms below about 0.009 % C at 1 atm.
Method and article reviewed by FireCAD engineering on 17 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.
Sources
Fruehan (ed.), The Making, Shaping and Treating of Steel, 11th ed., Steelmaking and Refining Volume (AISE Steel Foundation, 1998), sec. 2.4.2.2, eq. 2.4.13 and sec. 2.4.5, eq. 2.4.31