Worked example
Example: Illustrative 950 C for 10 h, 0.2 % C steel. The inputs, in the units selected above:
| Input | Value |
|---|---|
| Surface carbon (wt %) | 1.0000 - |
| Initial carbon (wt %) | 0.20000 - |
| Diffusion pre-exponential | 23.000 mm²/s |
| Activation energy | 148.00 kJ/mol |
| Temperature | 950.00 °C |
| Time | 10.000 h |
| Depth of interest | 0.50000 mm |
| Carbon level for the depth output (wt %) | 0.40000 - |
Applying the formula below gives:
| Result | Value |
|---|---|
| Diffusion coefficient | 1.1003e-05 mm²/s |
| Diffusion length | 1.2587 mm |
| Carbon at the depth (wt %) | 0.65942 |
| Depth to the carbon level | 1.0239 mm |
Open this example in the calculator and change any input.
Formula
\(C(x) = C_s - (C_s - C_0)\,\mathrm{erf}\frac{x}{2\sqrt{Dt}}, \quad D = D_0e^{-Q/RT}\)
Variables
| Symbol | Meaning | SI unit |
|---|---|---|
| \(C_s\) | Surface carbon (wt %) | - |
| \(C_0\) | Initial carbon (wt %) | - |
| \(D_0\) | Diffusion pre-exponential | m²/s |
| \(Q\) | Activation energy | J/mol |
| \(T\) | Temperature | K |
| \(t\) | Time | s |
| \(x\) | Depth of interest | m |
| \(C_x\) | Carbon level for the depth output (wt %) | - |
| \(D\) | Diffusion coefficient | m²/s |
| \(2\sqrt{Dt}\) | Diffusion length | m |
| \(C(x)\) | Carbon at the depth (wt %) | - |
| \(x_C\) | Depth to the carbon level | m |
Method and standards
Fick profile.
Where it is used
- Carburising cycle design.
- Decarburisation in forging and heat treatment.
Common mistakes
- Using ferrite diffusion data at austenitising temperatures.
- Expecting the surface carbon to be reached instantly in practice.
Assumptions and limits
- Semi-infinite plate; constant D and surface carbon.
References
- Fick's second law
- constant surface concentration
Questions and answers
Why does depth go with √t?
Diffusion distance scales with √(Dt): doubling the depth needs four times the time.
How does temperature help so much?
D rises exponentially with temperature; carburising 50 °C hotter can halve the cycle.
What do the defaults represent?
An illustrative 0.2 % C steel carburised at 950 °C for 10 hours with 1.0 % surface carbon, checked at 0.5 mm and for the depth to 0.4 % C.
Method and article reviewed by FireCAD engineering on 17 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.
Sources
Callister and Rethwisch, Materials Science and Engineering, 9th ed. (Wiley, 2014), ch. 5