Worked example
Example: Illustrative steel, Ms 350 C to 20 C. The inputs, in the units selected above:
| Input | Value |
|---|---|
| Martensite start temperature | 350.00 °C |
| Quench (lowest) temperature | 20.000 °C |
| Rate constant (1/K) | 0.011000 - |
Applying the formula below gives:
| Result | Value |
|---|---|
| Martensite fraction | 97.348 % |
| Retained austenite | 2.6516 % |
| Temperature for 90 % martensite | 140.67 °C |
| Temperature for 99 % martensite | -68.652 °C |
Open this example in the calculator and change any input.
Formula
\(f_m = 1 - e^{-\alpha_m(M_s - T_q)}, \quad T_{90} = M_s - \frac{\ln 10}{\alpha_m}\)
Variables
| Symbol | Meaning | SI unit |
|---|---|---|
| \(M_s\) | Martensite start temperature | K |
| \(T_q\) | Quench (lowest) temperature | K |
| \(\alpha_m\) | Rate constant (1/K) | - |
| \(f_m\) | Martensite fraction | - |
| \(f_\gamma\) | Retained austenite | - |
| \(T_{90}\) | Temperature for 90 % martensite | K |
| \(T_{99}\) | Temperature for 99 % martensite | K |
Method and standards
Martensite fraction.
Where it is used
- Choosing sub-zero treatment for tool and bearing steels.
- Heat treatment simulation inputs.
Common mistakes
- Using it above M_s or for steels that form bainite first.
- Taking α as universal for high-alloy steels.
Assumptions and limits
- Fully austenitised steel; no prior bainite or ferrite; athermal kinetics.
References
- Koistinen–Marburger relation
Questions and answers
Why does high-carbon steel keep austenite after quenching?
Its M_s is low, so room temperature is not far enough below it to transform everything.
Does holding at the quench temperature form more martensite?
Not appreciably: the transformation depends on undercooling, not time.
What do the defaults represent?
An illustrative steel with M_s = 350 °C quenched to 20 °C.
Method and article reviewed by FireCAD engineering on 17 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.
Sources
Koistinen and Marburger, A General Equation Prescribing the Extent of the Austenite-Martensite Transformation, Acta Metallurgica 7 (1959)