Carburising Case Depth vs Time and Temperature (Harris)

Total case depth of gas or pack carburised steel after a time at temperature, and the time for a wanted depth, by the Harris diffusion equation.

Refinery and petrochemicalChemical and fertiliser

Inputs

Examples: 925 °C for 4 h, 1 mm wanted900 °C for 8 h, 1.5 mm wanted950 °C for 2 h, 0.8 mm wanted

Results

Total case depth for a saturated carbon potential at the surface; effective case depth (to a hardness such as 50 HRC) is smaller. Boost–diffuse cycles need their own calculation.

Total case depth after the time1.2558mm
Carburising factor (depth after 1 h)0.62788mm
Time for the wanted depth2.5365h

Download PDF CSV Link to this result Compare another case

Log in to save calculations to your dashboard.

Worked example

Example: 925 °C for 4 h, 1 mm wanted. The inputs, in the units selected above:

InputValue
Carburising temperature925.00 °C
Time at temperature4.0000 h
Case depth wanted1.0000 mm

Applying the formula below gives:

ResultValue
Total case depth after the time1.2558 mm
Carburising factor (depth after 1 h)0.62788 mm
Time for the wanted depth2.5365 h

Open this example in the calculator and change any input.

Formula

\(d = \frac{31.6 \sqrt{t}}{10^{6700/T}} \ \ (\text{in, h, °R}) \;=\; \frac{803 \sqrt{t}}{10^{3722/T}} \ \ (\text{mm, h, K})\)

\(t_t = \left(\frac{d_t}{k}\right)^2\)

Variables

Symbol Meaning SI unit
\(T\) Carburising temperature K
\(t\) Time at temperature s
\(d_t\) Case depth wanted m
\(d\) Total case depth after the time m
\(k\) Carburising factor (depth after 1 h) m
\(t_t\) Time for the wanted depth s

Method and standards

Harris's diffusion relation: case depth grows with the square root of time, with a temperature factor of Arrhenius form.

Where it is used

  • Planning carburising cycles for gears and shafts.
  • Checking a supplier's quoted case depth.
  • Comparing temperatures for productivity.

Common mistakes

  • Confusing total and effective case depth.
  • Using furnace set point instead of part temperature.
  • Ignoring the low carbon potential at the start of a cycle.

Assumptions and limits

  • Saturated carbon potential at the surface; plain carbon and low-alloy steels.

References

  • F.E. Harris (1943)
  • Metal Progress 44
  • total case depth

Questions and answers

What case does 4 h at 925 °C give?

About 1.26 mm total case: the carburising factor is 0.63 mm per √h at that temperature.

How long for 1 mm?

About 2.5 hours at 925 °C: depth goes with the square root of time, so doubling the depth takes four times as long.

Is this effective case depth?

No, total case; effective case (to about 50 HRC) is smaller, often about two-thirds.

Method and article reviewed by FireCAD engineering on 12 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.

Related calculators

Free engineering calculators: every page computes in SI and converts to your units. Results are for engineering estimation; verify critical designs against the referenced standards.

Rejoining the server...

Rejoin failed... trying again in seconds.

Failed to rejoin.
Please retry or reload the page.

The session has been paused by the server.

Failed to resume the session.
Please retry or reload the page.