FireCADCalc

Martensite Fraction on Quenching (Koistinen–Marburger)

Martensite fraction and retained austenite after quenching steel to a temperature below Ms, and the temperatures for 90 % and 99 % martensite.

Inputs

Examples: Illustrative steel, Ms 350 C to 20 CHigh-carbon steel, Ms 180 C to 20 CSub-zero treatment to -80 C

Accepted: -173.15 to 726.85 °C
Accepted: -269.15 to 726.85 °C
Accepted: 0.0001 to 0.1

Results

Martensite forms athermally: the fraction depends on how far below M_s the steel is cooled, not on time. Koistinen and Marburger fitted f_m = 1 − exp[−α(M_s − T_q)] with α = 0.011/K for plain carbon and low-alloy steels (any austenite that does not become bainite or ferrite first). High-carbon and high-alloy steels with low M_s retain austenite at room temperature, which a sub-zero treatment converts. Use M_s from the Andrews calculator.

Martensite fraction82.796%
Retained austenite17.204%
Temperature for 90 % martensite-29.326°C
Temperature for 99 % martensite-238.65°C

Download PDF CSV Link to this result Compare another case

Log in to save calculations to your dashboard.

Worked example

Example: Illustrative steel, Ms 350 C to 20 C. The inputs, in the units selected above:

InputValue
Martensite start temperature350.00 °C
Quench (lowest) temperature20.000 °C
Rate constant (1/K)0.011000 -

Applying the formula below gives:

ResultValue
Martensite fraction97.348 %
Retained austenite2.6516 %
Temperature for 90 % martensite140.67 °C
Temperature for 99 % martensite-68.652 °C

Open this example in the calculator and change any input.

Formula

\(f_m = 1 - e^{-\alpha_m(M_s - T_q)}, \quad T_{90} = M_s - \frac{\ln 10}{\alpha_m}\)

Variables

Symbol Meaning SI unit
\(M_s\) Martensite start temperature K
\(T_q\) Quench (lowest) temperature K
\(\alpha_m\) Rate constant (1/K) -
\(f_m\) Martensite fraction -
\(f_\gamma\) Retained austenite -
\(T_{90}\) Temperature for 90 % martensite K
\(T_{99}\) Temperature for 99 % martensite K

Method and standards

Martensite fraction.

Where it is used

  • Choosing sub-zero treatment for tool and bearing steels.
  • Heat treatment simulation inputs.

Common mistakes

  • Using it above M_s or for steels that form bainite first.
  • Taking α as universal for high-alloy steels.

Assumptions and limits

  • Fully austenitised steel; no prior bainite or ferrite; athermal kinetics.

References

  • Koistinen–Marburger relation

Questions and answers

Why does high-carbon steel keep austenite after quenching?

Its M_s is low, so room temperature is not far enough below it to transform everything.

Does holding at the quench temperature form more martensite?

Not appreciably: the transformation depends on undercooling, not time.

What do the defaults represent?

An illustrative steel with M_s = 350 °C quenched to 20 °C.

Method and article reviewed by FireCAD engineering on 17 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.

Sources

Koistinen and Marburger, A General Equation Prescribing the Extent of the Austenite-Martensite Transformation, Acta Metallurgica 7 (1959)

Related calculators

Free engineering calculators: every page computes in SI and converts to your units. Results are for engineering estimation; verify critical designs against the referenced standards.

Rejoining the server...

Rejoin failed... trying again in seconds.

Failed to rejoin.
Please retry or reload the page.

The session has been paused by the server.

Failed to resume the session.
Please retry or reload the page.