FireCADCalc

Bogue Potential Phase Composition of Clinker (C3S, C2S, C3A, C4AF)

Potential clinker phases C3S, C2S, C3A and C4AF from the oxide analysis by Bogue's method, with free lime deducted, and the liquid-forming phases.

Inputs

Examples: Ordinary Portland clinkerDuda Table 2.2 clinkerSulphate-resisting clinker, low C3A

Results

Potential, not actual, phase contents: Bogue assumes equilibrium crystallisation and pure phases. Free lime is deducted from CaO; SO₃ and minor oxides are not deducted here.

Tricalcium silicate (alite)65.017%
Dicalcium silicate (belite)13.853%
Tricalcium aluminate8.6881%
Tetracalcium aluminoferrite9.9202%
Alumina ratio1.6442
Aluminate and ferrite phases (flux)18.608%

Download PDF CSV Link to this result Compare another case

Log in to save calculations to your dashboard.

Worked example

Example: Ordinary Portland clinker. The inputs, in the units selected above:

InputValue
CaO66.000 %
SiO₂21.500 %
Al₂O₃5.2000 %
Fe₂O₃3.2000 %
Free lime1.0000 %

Applying the formula below gives:

ResultValue
Tricalcium silicate (alite)61.705 %
Dicalcium silicate (belite)15.090 %
Tricalcium aluminate8.3656 %
Tetracalcium aluminoferrite9.7376 %
Alumina ratio1.6250
Aluminate and ferrite phases (flux)18.103 %

Open this example in the calculator and change any input.

Formula

\(C_3S = 4.071C - 7.600S - 6.718A - 1.430F, \quad C_2S = 2.867S - 0.7544\,C_3S, \quad C_3A = 2.650A - 1.692F, \quad C_4AF = 3.043F\)

Variables

Symbol Meaning SI unit
\(C\) CaO -
\(S\) SiO₂ -
\(A\) Al₂O₃ -
\(F\) Fe₂O₃ -
\(CaO_f\) Free lime -
\(C_3S\) Tricalcium silicate (alite) -
\(C_2S\) Dicalcium silicate (belite) -
\(C_3A\) Tricalcium aluminate -
\(C_4AF\) Tetracalcium aluminoferrite -
\(A/F\) Alumina ratio -
\(C_3A + C_4AF\) Aluminate and ferrite phases (flux) -

Method and standards

Bogue's calculation.

Where it is used

  • Clinker quality control.
  • Cement type selection (sulphate resisting, low heat).

Common mistakes

  • Using total CaO with high free lime.
  • Applying it below an alumina ratio of 0.64.

Assumptions and limits

  • Equilibrium cooling; pure phases.

References

  • Duda
  • Cement Data Book
  • Vol. 1
  • 3rd ed. (Bauverlag / Macdonald and Evans, 1985)
  • sec. 1.6 (Bogue)

Questions and answers

Why 'potential' composition?

Bogue's phases assume complete equilibrium and pure compounds; real clinker minerals hold foreign ions and the microscope often finds more alite.

What if the alumina ratio is below 0.64?

Then all alumina is in the ferrite phase, no C3A forms and a different set of equations (C4AF + C2F) applies.

What do the defaults represent?

A typical ordinary Portland clinker: 66.0 % CaO, 21.5 % SiO₂, 5.2 % Al₂O₃, 3.2 % Fe₂O₃, 1.0 % free lime.

Method and article reviewed by FireCAD engineering on 17 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.

Related calculators

Free engineering calculators: every page computes in SI and converts to your units. Results are for engineering estimation; verify critical designs against the referenced standards.

Rejoining the server...

Rejoin failed... trying again in seconds.

Failed to rejoin.
Please retry or reload the page.

The session has been paused by the server.

Failed to resume the session.
Please retry or reload the page.