Worked example
Example: 4340-type. The inputs, in the units selected above:
| Input | Value |
|---|---|
| Carbon (wt %) | 0.40000 - |
| Manganese (wt %) | 0.75000 - |
| Nickel (wt %) | 1.8000 - |
| Chromium (wt %) | 0.80000 - |
| Molybdenum (wt %) | 0.25000 - |
Applying the formula below gives:
| Result | Value |
|---|---|
| Martensite start temperature | 303.58 °C |
Open this example in the calculator and change any input.
Formula
\(M_s(°C) = 539 - 423C - 30.4Mn - 17.7Ni - 12.1Cr - 7.5Mo\)
Variables
| Symbol | Meaning | SI unit |
|---|---|---|
| \(C\) | Carbon (wt %) | - |
| \(Mn\) | Manganese (wt %) | - |
| \(Ni\) | Nickel (wt %) | - |
| \(Cr\) | Chromium (wt %) | - |
| \(Mo\) | Molybdenum (wt %) | - |
| \(M_s\) | Martensite start temperature | K |
Method and standards
Andrews linear.
Where it is used
- Heat treatment of shafts, gears and bolts.
- Weld cracking discussions.
Common mistakes
- Weight % as fractions.
- High-alloy steels outside the range.
Assumptions and limits
- Low-alloy steels, full austenitisation. Compositions far outside Andrews' data that would give a temperature below absolute zero are rejected.
- Compositions are entered as plain weight-per-cent numbers (0.4 for 0.4 % C), unlike the Andrews critical temperatures calculator, which takes them as percentages; the inputs are kept as they are so saved links keep their meaning.
References
- Andrews (1965)
- J. Iron Steel Inst. 203: Ms (°C) = 539 − 423C − 30.4Mn − 17.7Ni − 12.1Cr − 7.5Mo
Questions and answers
4340-type steel (0.4 C, 0.75 Mn, 1.8 Ni, 0.8 Cr, 0.25 Mo)?
Ms about 304 °C.
Why does carbon dominate?
It stabilises austenite strongly: about 42 °C lower per 0.1 % C.
Use?
Set quench and austempering temperatures and judge cracking risk.
Method and article reviewed by FireCAD engineering on 12 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.