Worked example
Example: Illustrative 6 mm test. The inputs, in the units selected above:
| Input | Value |
|---|---|
| Wall thickness in the test | 6.0000 mm |
| Casting time in the test | 30.000 min |
| Wall thickness wanted | 8.0000 mm |
| Time for which to predict thickness | 60.000 min |
Applying the formula below gives:
| Result | Value |
|---|---|
| Casting rate constant L²/t | 1.2000 |
| Time for the wanted thickness | 53.333 min |
| Thickness after the prediction time | 8.4853 mm |
Open this example in the calculator and change any input.
Formula
\(L^2 = K t, \quad t_2 = t_1\left(\frac{L_2}{L_1}\right)^2\)
Variables
| Symbol | Meaning | SI unit |
|---|---|---|
| \(L_1\) | Wall thickness in the test | m |
| \(t_1\) | Casting time in the test | s |
| \(L_2\) | Wall thickness wanted | m |
| \(t\) | Time for which to predict thickness | s |
| \(K\) | Casting rate constant L²/t | - |
| \(t_2\) | Time for the wanted thickness | s |
| \(L(t)\) | Thickness after the prediction time | m |
Method and standards
Slip casting.
Where it is used
- Sanitaryware, tableware and technical ceramics.
- Pressure casting set-up.
Common mistakes
- Using a linear rate.
- Testing with a wet or different mould.
Assumptions and limits
- Constant slip and mould conditions.
References
- Parabolic filtration law of slip casting
Questions and answers
How long for an 8 mm wall if 6 mm takes 30 min?
30 × (8/6)² = 53 min.
Why does casting slow down?
The cast layer itself resists the flow of water into the mould, more as it thickens.
What do the defaults represent?
A test casting of 6 mm in 30 min, predicted for 8 mm and for 60 min.
Method and article reviewed by FireCAD engineering on 17 November 2026. Every result is checked against an independent calculation on each release: how we verify our calculators.
Sources
Reed, Principles of Ceramics Processing, 2nd ed. (Wiley, 1995)